Technical guide with sources · ROLL Lab
Paper core crush strength: flat crush, radial crush and ID stiffness
On this page · calculators
The three tests, and why they give different numbers
| Test | How it is done | Result |
|---|---|---|
| Flat crush ISO 11093-9, CCTI T-108 | A 100 mm sample crushed between two parallel plates at 50–65 mm/min up to the first maximum | Force per unit length: kN/m (100 N/100 mm = 1 kN/m) |
| Radial crush CCTI T-158 / T-159 | The core sits in a chamber where pressure rises uniformly over the whole surface; T-158 with steel balls and ID reduction measured, T-159 with an inflatable bladder | Failure pressure in bar |
| ID stiffness | How much pressure reduces the inside diameter by 0.1 mm | bar / 0.1 mm: decides whether the roll comes off the shaft |
Plates or vice?
The two values correlate poorly: cores with the same flat crush can have very different radial crush, and vice versa. The reason is geometric: film does not crush the core between two plates, it squeezes it from every side.
What film does to a core
Film is elastic: after winding it keeps shrinking and each wrap squeezes the ones below. The core receives a uniform pressure which, in practice, ranges from about 5 to over 100 bar. Inside diameter, outside diameter and length all move together; the inside diameter is the critical one, because if it closes too much the roll stays on the winder or will not go onto the unwinder.
The pressure depends on variables upstream of the core: film gauge, lay-on roller, number of wraps, tension, film type and formulation, age of the roll, environment. Down-gauging (thinner film for the same holding force) raises the radial pressure.

When it fails: often not in front of you
| Film | Typical failure |
|---|---|
| Cast | within 72 hours |
| Blown | within 7 to 14 days |
The film type decides when the core fails; the ratio between pressure and radial strength decides whether it fails. A core that comes off the line looking fine is not yet approved: recheck at 72 hours and at 14 days.
The crush curve: paper and plastic are not measured the same way
Force against deflection
On paper (ISO 11093-9) the figure is the peak: the force rises, the wall gives way, the force drops and settles. The standard does not fix the deflection at the peak, though, so two cores with the same value can reach it at 3% or at 10% deflection. Plastic has no peak: you read the force at 3% of the diameter (ISO 9969), and the maximum load is about 2.2 times that force. Write a load specification around the weakest core in the comparison, not the highest curve.
The strength levers
- Wall and board grade: the grade of the board matters more than its density. Denser board weighs more; what shifts strength is the grade.
- Moisture: the strongest lever and the only one that changes after delivery. One extra point costs about 3.6% of flat crush, 7.1% of radial crush and 12.3% of ID stiffness (moisture guide).
- Diameter: with the same wall, a 6" core has lower radial strength than a 3": in published tests with a 10 mm wall, 28.8 bar against 39.2 (−27%).
- Core construction: strip width and winding angle, board type (cylinder or Fourdrinier machine) and adhesive type shift radial strength even at the same flat crush. These are the manufacturer’s choices: ask about them if you change supplier.
- Age: dynamic load capacity improves with seasoning; rush deliveries leave before the strength has fully developed.
Bending, torque and upright load
Flat crush and radial crush do not tell the whole story. A wide reel supported at its ends makes the core work like a beam: bending strength and flexural modulus matter (ISO 11093-6 and -7) and, on fast machines, the critical speed (the formula is on the paper mill page). The toothed chucks that start and brake the reel transmit torque to the ends: with a weak wall the paper tears and the core spins freely. Finally, reels stored upright load the core axially.
None of these strengths can be derived from flat crush. If one applies to your line, write it into the specification with its test method; the terms are explained in the glossary.
A specification that really works
For a film core: minimum radial crush in bar with the method stated (T-158 or T-159), with a margin over the pressure measured on the line; flat crush to ISO 11093-9 as a production check; maximum moisture on delivery measured in an oven; inside diameter with ISO 13542 tolerance, measured at three points. Estimate pressure and margin in the radial duel.
Frequently asked questions
What is the flat crush of a paper core?
It is the resistance to flat crushing: a 100 mm sample is squeezed between two parallel plates until it first gives way. The standard is ISO 11093-9 (published in the UK as BS ISO 11093-9; the US equivalent is CCTI T-108). The result is given in kN/m or N/100 mm.
What is the difference between flat crush and radial crush?
Flat crush squeezes the core between two plates, along a line. Radial crush squeezes it with uniform pressure over the whole surface, as a wound film does, and is measured in bar (CCTI T-158 with steel balls, T-159 with an inflatable bladder). The two values correlate poorly: for film rolls, radial strength is what counts.
What is ID stiffness?
It is the pressure in bar needed to reduce the inside diameter by 0.1 mm. It is not a failure but a stiffness, and it decides whether the roll comes off the shaft. It is also the property moisture degrades most: about −12% for each extra point of moisture, according to published studies.
How do you convert N/100 mm, kN/m and lbf/in?
100 N/100 mm = 1 kN/m = 1 N/mm. 1 lbf/in = 175.1 N/m = 17.5 N/100 mm. So 1,500 N/100 mm = 15 kN/m ≈ 85.7 lbf/in. The ROLL Lab converter handles every conversion.
How much pressure does a film roll put on its core?
In practice, from about 5 to over 100 bar. It depends on winding tension, film type and gauge, number of wraps, lay-on roller and time. Film keeps shrinking after winding and keeps squeezing: under cast film, cores typically fail within 72 hours; under blown film, within 7 to 14 days.
What affects the strength of a paper core?
Wall thickness, board grade, diameter, moisture, strip width and winding angle, adhesive type (silicate or dextrin) and the age of the core. Moisture is the strongest lever, and the only one that keeps changing after delivery.
Why does the same standard give different numbers for paper and plastic?
For paper (ISO 11093-9) you measure the force at first failure, the peak. Plastic has no peak: it goes oval and keeps resisting, so you measure the force at a set deflection, 3% of the diameter (ISO 9969). On plastic, the maximum load is about 2.2 times the strength at 3%.
Is flat crush enough in a specification?
No, not if the core goes under a film roll. Flat crush barely reacts to the variables that drive radial strength: across moisture and core construction it moves 3 to 25 times less than ID stiffness. A useful specification also states the minimum radial crush in bar and the test method.
Sources
- ISO 11093-9:2006 (rev. 2019) — Determination of flat crush resistance
- UNI 10328-7 — Italian standard, determination of compressive strength
- CCTI T-108; CCTI T-158 (steel balls, 2011); CCTI T-159 (inflatable bladder)
- ISO 9969:2007 — Thermoplastics pipes, ring stiffness
- Gerhardt, ASME Journal of Engineering Materials and Technology 112 (1990) 144–150
- ROLL Lab calculation
Find your core → Find a core maker